Ductile Cast Iron Pump Housings

What Is Ductile Cast Iron?

Contents show

1. Introduction

Ductile cast iron, often called nodular cast iron or spheroidal graphite iron.

In 1948, Keith Millis discovered that adding a small amount of magnesium to molten iron created nearly spherical graphite nodules rather than flakes.

This breakthrough yielded ductile cast iron (DI), which combines castability and economy with markedly improved tensile strength and elongation.

This article delves into ductile cast iron’s fundamental nature, its chemistry and microstructure, mechanical performance, processing routes, corrosion resistance,

key applications, advantages and limitations, and comparisons to alternative materials.

2. What Is Ductile Cast Iron?

Ductile cast iron (DI) qualifies as a cast iron family characterized by spheroidal (nodular) graphite inclusions uniformly dispersed in a metallic matrix.

In contrast to gray iron’s flake-shaped graphite, prone to stress concentration, DI’s graphite nodules arrest crack propagation, enabling ductile behavior.

Ductile cast iron
Ductile cast iron

Ductile iron bridges the performance gap between gray iron and low-alloy steel.

Manufacturers exploit ductile cast iron for components under cyclic loads, where both high strength and impact resistance matter.

Moreover, DI’s machinability and near-net-shape capability reduce downstream processing costs.

3. Chemical Composition and Alloy Systems

Base Composition: Fe–C–Si–Mn–P–S

Ductile cast iron’s foundation lies in a typical gray iron charge—iron (Fe), carbon (C), silicon (Si), manganese (Mn), phosphorus (P), and sulfur (S).

A representative chemical range for a common grade (ASTM A536 65-45-12) might be:

  • C: 3.5 – 3.8 wt %
  • Si: 2.2 – 2.8 wt %
  • Mn: 0.1 – 0.4 wt %
  • P: ≤ 0.08 wt %
  • S: ≤ 0.025 wt %

High silicon (≥ 2 wt %) promotes graphite formation rather than cementite, while low sulfur (< 0.025 wt %) prevents excessive inclusions that interfere with nodule formation.

Nodulizing Elements: Magnesium (Mg), Cerium (Ce), and Rare Earths (RE)

Nodularity in ductile cast iron arises from adding magnesium—typically 0.03% – 0.05% Mg—to molten iron.

Foundries introduce magnesium via Mg–Fe master alloys or cored wires. Magnesium’s strong affinity for sulfur forms MgS, so they tightly control sulfur to remain under 0.025%.

Many foundries also add 0.005 – 0.01 wt% cerium or rare-earth elements to refine nodule shape and size, improving mechanical consistency, especially in thick sections.

These RE additions further reduce sensitivity to variations in sulfur and oxygen.

Additional Alloying: Copper (Cu), Nickel (Ni), Molybdenum (Mo), Chromium (Cr)

To tailor strength, toughness, or corrosion resistance, foundries incorporate secondary alloying elements:

  • Copper (Cu): 0.2 – 0.5 wt % boosts pearlite formation, raising strength by 10 – 20 %.
  • Nickel (Ni): 0.5 – 1.5 wt % enhances low-temperature toughness and corrosion resistance.
  • Molybdenum (Mo): 0.2 – 0.4 wt % improves hardenability and creep resistance for higher-temperature service.
  • Chromium (Cr): 0.2 – 0.5 wt % confers mild corrosion resistance and firmer microstructure.

Typically, ductile cast iron grades remain within 1 – 2 wt % of combined Cu + Ni + Mo + Cr, ensuring cost-efficiency while meeting performance targets.

Standards and Grades

  • ASTM A536 (USA): 60-40-18, 65-45-12, 80-55-06 grades.
  • ISO 1083 (Europe): EN-GJS-400-15, GJS-450-10, GJS-700-2.
  • DIN EN 1563 (Germany): GG-25, GS-32, GS-45 equivalents.

4. Physical and Mechanical Properties of Ductile Cast Iron

Ductile Iron Sand Casting Auto Parts
Ductile Iron Sand Casting Auto Parts

Tensile Strength, Yield Strength, and Ductility

Ductile iron’s signature is its combination of high strength and appreciable ductility:

Grade UTS (MPa) Yield (0.2% offset, MPa) Elongation (%) Matrix
60-40-18 (A536) 400 – 550 245 – 415 10 – 18 Ferritic–Pearlitic
65-45-12 (A536) 450 – 650 275 – 450 8 – 12 Pearlitic–Ferritic
80-55-06 (A536) 700 – 900 415 – 620 3 – 6 Fully Pearlitic

By contrast, standard gray iron yields only 200 – 300 MPa tensile strength with virtually no elongation.

Because DI’s graphite nodules blunt crack initiation, elongation leaps into the double digits for lower-strength grades.

Hardness and Wear Resistance

Ductile iron’s hardness spans 170 – 320 HB, depending on grade and matrix:

  • A ferritic grade (60-40-18) delivers around 170 HB, suitable for general-purpose castings (manifolds, frames).
  • A high-strength pearlitic grade (80-55-06) achieves 260 – 320 HB, rivaling low-alloy steel in wear resistance for gears, sprockets, and pump impellers.

When wear resistance is critical, manufacturers often select austempered ductile iron (ADI),

which reaches 300 – 450 HB after heat treatment, balancing hardness with residual toughness.

Fatigue Life and Impact Toughness

Ductile iron’s spherical graphite significantly enhances fatigue performance:

  • Fatigue limit typically stands at ≈ 40% of UTS. For a 65-45-12 grade (UTS ≈ 500 MPa), fatigue endurance reaches 200 MPa at 10⁷ cycles under reversed bending.
  • Impact toughness (Charpy V-notch at 20 °C) ranges from 15 – 60 J, depending on grade. Lower-strength, ferritic-rich grades absorb up to 60 J, whereas fully pearlitic grades dip to 15 J.

These values surpass gray iron (10 – 20 J) and approach low-alloy steel, making ductile cast iron ideal for high-cycle applications like crankshafts and connecting rods.

Modulus of Elasticity and Damping Capacity

Unlike gray iron’s 100 – 120 GPa modulus, ductile iron’s modulus measures 170 – 200 GPa, roughly matching that of low-alloy steel.

This high stiffness, combined with damping capacity around 0.005 to 0.010 (logarithmic decrement),

ensures that ductile cast iron parts resist deflection under load while attenuating vibrations—beneficial in engine components and machinery bases.

Thermal Conductivity and Coefficient of Thermal Expansion

Property Ductile Iron Gray Iron Steel (A36)
Thermal Conductivity (W/m·K) 35 – 50 35 – 45 45
Coefficient of Thermal Expansion (×10⁻⁶/°C) 12 – 13 10 – 12 11 – 13

Ductile iron’s thermal conductivity parallels that of gray iron and steel, enabling efficient heat dissipation in engine blocks and brake drums.

Its thermal expansion coefficient (~ 12 × 10⁻⁶/°C) aligns closely with steel, simplifying multi-material design.

5. Corrosion Behavior and Environmental Resistance

Passive Films and Surface Oxidation

Ductile iron forms an iron oxide (Fe₃O₄/Fe₂O₃) film when exposed to oxygen. This passive layer slows further oxidation in mild environments.

Alloying additions like 0.5 – 1.5% Ni or 0.2 – 0.5% Cr improve corrosive performance by stabilizing the passive film.

Unlike gray iron—which may develop pitting—DI’s matrix can better resist localized attack, especially when coated.

Sand Casting Ductile Cast Iron
Sand Casting Ductile Cast Iron

Comparative Corrosion Rates vs. Gray Iron and Steel

Environment DI (Uncoated, mm/y) Gray Iron (mm/y) Mild Steel (mm/y)
Fresh Water 0.05 – 0.10 0.10 – 0.15 0.20 – 0.30
Seawater 0.20 – 0.35 0.40 – 0.60 0.50 – 1.00
Acidic (pH 3 – 4) 0.15 – 0.25 0.30 – 0.40 0.50 – 1.00
Alkaline (pH 9 – 10) 0.02 – 0.05 0.05 – 0.08 0.10 – 0.20

In each case, ductile cast iron’s corrosion rate remains roughly 50% that of gray iron and 30–40% that of mild steel.

Applying epoxy or polyurethane coatings reduces DI’s corrosion to < 0.01 mm/year in aggressive environments.

When buried or submerged, designers employ zinc or aluminum sacrificial anodes to protect uncoated ductile cast iron pipelines and fittings.

Corrosion Control: Coatings, Cathodic Protection, and Material Selection

  • Coatings: High-build epoxy (200 µm) or flame-sprayed zinc/aluminum layers extend service life in marine or chemical processing plants.
  • Cathodic Protection: Impressed current or sacrificial anodes maintain ductile cast iron pipe integrity in underground or underwater installations.
  • Material Selection: In highly corrosive conditions (pH < 3 or chloride > 10 000 ppm), engineers specify Ni-alloyed DI or stainless steel instead of standard grades.

6. Manufacturing Processes of Ductile Cast Iron

Molding Methods: Sand Casting, Shell Molding, and Investment Casting

  • Green Sand Casting remains the predominant method. Foundries pack silica sand with clay or chemical binders into flasks around patterns.
    Sand molds accommodate risers, cores, and gating systems tailored for DI’s fluidity. Typical minimum section thickness hovers around 6 – 8 mm to avoid shrinkage defects.
  • Shell Molding uses a heated resin-coated sand mixture pressed around a heated metal pattern.
    This process yields surface finishes of Ra = 1–3 µm and tolerances ± 0.3 mm, at a cost premium of ~ 20 % over green sand.
  • Investment Casting (Lost Wax) facilitates thin sections (down to 3 mm) and complex geometries with tolerances ± 0.1 mm.
    However, ductile cast iron investment casts command 2–3× the cost of sand-cast equivalents, restricting usage to low-volume or intricate parts.
Investment Casting Ductile Cast Iron Exhaust Manifold
Investment Casting Ductile Cast Iron Exhaust Manifold

Heat Treatment: Annealing, Normalizing, Austempering (ADI)

Heat treatment tailors DI’s matrix and mechanical performance:

  • Annealing: Slow cooling from 900 °C down to room temperature produces a fully ferritic matrix, maximizing ductility (~ 18 % elongation) and machinability (400 MPa UTS).
  • Normalizing: Heating to 900 – 920 °C followed by air cooling yields a balanced ferritic–pearlitic microstructure, offering UTS ≈ 450 MPa and 12 % elongation.
  • Austempering (ADI): The ductile cast iron casting undergoes solutionizing at 900 °C to dissolve carbides, then quenching into a salt bath at 250 – 375 °C for 1 – 4 hours.
    This produces a bainitic ferrite + carbon-enriched retained austenite structure.
    ADI grades range from 400 MPa to 1 400 MPa UTS, with elongations between 2 – 12 %, and exceptional fatigue performance (endurance limits up to 400 MPa).

Post-processing: Machining, Surface Finishing, Coating

  • Machining: ductile cast iron machines similarly to carbon steel. Typical turning speeds for 65-45-12 hover at 150–250 m/min with carbide tooling.
    Drill speeds range 50–100 m/min. Coolant lubrication prevents built-up edge. DI’s lack of flake graphite reduces tool chipping.
  • Surface Finishing:
    • Shot Blasting with steel grit (20–40 mesh) removes sand and provides a matte finish (Ra 2 – 5 µm).
    • Grinding/Polishing achieves Ra < 0.8 µm for sealing surfaces.
  • Coating:
    • Epoxy/Powder Coating: Deposits a 50–200 µm film to guard against corrosion in marine or industrial environments.
    • Metalizing (Zinc or Aluminum): Thermal spray applies a 100 – 150 µm sacrificial layer for buried or submerged parts.

7. What Is Austempered Ductile Iron (ADI)

Austempered Ductile Iron (ADI) represents a specialized subclass of ductile cast iron that offers an exceptional combination of strength, ductility, and fatigue resistance.

Unlike conventional ductile iron—which typically has a ferritic–pearlitic or fully pearlitic matrix,

ADI’s unique microstructure consists of fine bainitic ferrite plates immersed in a matrix of carbon-enriched retained austenite.

This microstructure arises from a three-step heat-treatment process: solutionizing, quenching to an intermediate temperature, and austempering.

Once completed, austempered ductile iron delivers tensile strengths as high as 1 400 MPa (in the ADI 900-650 grade) while preserving elongation in the 2 – 5% range.

Austempered Ductile Iron Ball Valve
Austempered Ductile Iron Ball Valve

Austempered Ductile Iron Production Route: Solutionizing, Quenching, and Austempering

The key steps in austempered ductile iron processing include:

  1. Solutionizing: Heat the ductile iron casting to 880 – 920 °C for 1–2 hours to dissolve carbides and homogenize carbon.
  2. Quenching: Transfer to a salt-bath at 250 – 375 °C. This intermediate temperature prevents martensite.
  3. Austempering: Hold until the matrix transforms into bainitic ferrite plus carbon-enriched retained austenite—typically 1–4 hours, depending on section thickness.
  4. Cooling: Air or oil quench to room temperature, locking in the bainitic microstructure.

Austempered Ductile Iron Microstructure: Bainitic Ferrite and Carbon-Enriched Austenite

ADI’s microstructure consists of:

  • Bainitic Ferrite Needles: Extremely fine α-iron ferrite blades that nucleate at austenite boundaries.
  • Retained Austenite: Carbon-rich austenite films that remain stable at room temperature, absorbing strain and increasing toughness.

This combination imparts a “transformation-toughening” effect: under applied stress, retained austenite transforms to martensite, locally strengthening the matrix.

Mechanical Advantages: High Strength–Ductility Balance, Fatigue Resistance

ADI Grade Tensile Strength (MPa) Yield Strength (MPa) Elongation (%) Brinell Hardness (HB) Fatigue Limit (MPa)
ADI 400-120 400 – 550 275 – 415 8 – 12 180 – 260 220 – 260
ADI 600-350 600 – 900 350 – 600 4 – 8 260 – 360 300 – 350
ADI 900-650 900 – 1 400 650 – 1 000 2 – 5 350 – 450 400 – 450

Compared to normalized ductile iron of similar composition, austempered ductile iron achieves up to 50% higher UTS while retaining 2 – 5% elongation.

Its fatigue endurance often exceeds 400 MPa, outperforming both gray iron and many alloy steels under reversed bending.

Typical Applications of Austempered Ductile Iron

Engineers use austempered ductile iron where high wear resistance, high strength, and reliable fatigue life matter:

  • Automotive: Gears, crankshafts, camshafts, and bearing cages.
  • Agricultural Machinery: Sprockets, wear plates, and roller shafts.
  • Oil & Gas: Downhole tools, pump shafts, and valve components requiring corrosion fatigue resistance.
  • Mining Equipment: Grates, crusher rolls, and mill liners subject to abrasive dust.

8. Applications of Ductile Cast Iron

Automotive Components: Crankshafts, Gears, Suspension Parts

Automakers leverage ductile cast iron’s high fatigue strength (≥ 250 MPa) and damping for crankshafts and camshafts in medium-duty engines.

Ductile iron gears endure shock loading while reducing noise. Control arms and steering knuckles benefit from DI’s stiffness (E ≈ 180 GPa) and impact resistance.

Pipeline and Fluid Handling: Pipes, Flanges, Pump Housings, Valve Bodies

Ductile cast iron pipe systems (EN-GJS-400-15) carry potable water or wastewater at pressures up to 25 bar.

Ductile iron valves and flanges resist cyclic pressure surges. Corrosion rates under alkaline or neutral pH remain minimal, making DI cost-effective compared to stainless steel in many routing applications.

Pipe flanges Ductile Cast Iron
Pipe flanges Ductile Cast Iron

Agricultural and Construction Equipment: Sprockets, Rollers, Frames

Field equipment components regularly face abrasive soils and high mechanical stresses.

Ductile cast iron sprockets and roller shafts achieve wear life exceeding 1 000 hours in severe environments,

while frames and structural castings minimize welding costs and improve fatigue life.

Energy Sector: Wind Turbine Housings, Gearbox Casings, Oilfield Components

Ductile cast iron’s high damping dampens torsional vibrations in wind turbine gearboxes, enhancing reliability.

Gearbox casings made from ADI reduce weight by 10% compared to steel and lower rotor inertia.

In oilfields, downhole tools and valve bodies endure corrosive brines while withstanding cyclic pressure up to 50 MPa.

Consumer Appliances and Tools

Ductile cast iron offers thermal mass and durability for cookware (Dutch ovens, cast-iron skillets).

Ductile iron socket wrenches and pipe-wrench bodies absorb shock without fracturing, extending tool life.

9. Core Pros and Cons of Ductile Cast Iron

Pros

Balanced Strength and Toughness:

Ductile iron delivers tensile strengths of 400–1 000 MPa and elongations of 2–18%, achieving a superior strength-to-weight ratio.

In automotive applications, for example, crankshaft weight can drop by 20–30% compared to steel counterparts.

Excellent Wear and Fatigue Resistance:

Spheroidal graphite nodules minimize stress concentrations, enabling fatigue limits up to 300 MPa.

This makes ductile iron ideal for gears, suspension components, and other parts under cyclic loading.

Superior Castability:

With a relatively low liquidus of 1 150–1 200 °C and good fluidity, ductile iron forms intricate geometries with minimal shrinkage (0.8–1.0%).

Casting and machining costs run 30–50% lower than comparable steel forgings.

Corrosion and Thermal Stability:

Graphite nodules provide a natural barrier against corrosion. After surface treatments, ductile cast iron fittings often last a century in soil or water environments.

It withstands temperatures up to 300 °C with a low coefficient of thermal expansion.

Cost-Effectiveness:

Raw materials are inexpensive, and melting requires relatively low energy.

Modern grades—such as austempered ductile iron—approach high-strength steel performance after heat treatment, offering significant overall cost savings.

Cons

Tight Process Control:

Achieving uniform nodules demands precise control of Mg/Ce levels and minimal sulfur/oxygen. Quality assurance adds to production complexity and cost.

Limited High-Temperature Performance:

Above 350 °C, strength declines sharply and graphite coarsening leads to creep.

Ductile iron is unsuitable for exhaust manifolds or other sustained high-heat components.

Machining Challenges:

High carbon content necessitates pre-heat or post-weld annealing to prevent cracking.

Graphite wears tools quickly, requiring carbide cutters and specialized machining strategies.

Lower Stiffness:

With a modulus of elasticity around 160–170 GPa (versus steel’s ≈ 210 GPa), ductile cast iron deforms more under load. Designers often need thicker sections to compensate.

Environmental Impact:

Melting and nodulizing consume significant energy and can generate pollutants.

Waste disposal must meet regulatory standards. In marine or acidic environments, ductile cast iron requires additional protective coatings.

10. Comparison with Other Materials

When engineers evaluate ductile cast iron (DI) for a particular application, they frequently weigh its properties against those of gray cast iron, malleable iron, steel alloys, aluminum, and bronze.

Gray Cast Iron vs. Ductile Iron

Metric Gray Cast Iron (GI) Ductile Cast Iron (DI)
Graphite Shape Flake Spheroidal (nodule)
Tensile Strength (MPa) 200 – 300 400 – 900
Elongation (%) < 2 % 3 – 18 %
Fatigue Endurance (MPa) 80 – 120 200 – 400
Impact Toughness (CVN, J) 10 – 20 15 – 60
Modulus of Elasticity (GPa) 100 – 120 170 – 200
Casting Cost vs. Steel Low 10 – 20 % higher than GI
Total Part Cost Lowest 20 – 30 % lower than GI (when strength-critical)
Typical Uses Machine beds, brake rotors, non-critical engine blocks Crankshafts, gears, suspension arms, pump housings

Malleable Iron vs. Ductile Iron

Metric Malleable Iron Ductile Cast Iron (DI)
Production Process White iron anneal (48–72 h @ 900 °C) Single-step nodulizing (Mg, RE)
Tensile Strength (MPa) 200 – 350 400 – 900
Elongation (%) 3 – 10 % 3 – 18 %
Heat Treatment Complexity Long, energy-intensive Nodulizing + optional heat treatment
Cycle Time 2–3 days (anneal) Hours (casting + nodulizing)
Cost (per kg) Moderate Lower (simpler process)
Typical Uses Hand tools, small brackets, fittings Automotive components, heavy machinery parts

Steel Alloys vs. Ductile Iron

Metric Low-Alloy Steel (e.g., 4140) Ductile Cast Iron (DI)
Density (g/cm³) ~ 7.85 ~ 7.20
Modulus of Elasticity (GPa) ~ 200 170 – 200
Tensile Strength (MPa) 800 – 1 100 400 – 900
Elongation (%) 10 – 15 % 3 – 18 %
Fatigue Limit (MPa) 300 – 400 200 – 400
Castability Poor (requires forging/machining) Excellent (near-net cast)
Machinability Rating 30 – 50 % (reference steel = 100) 60 – 80 %
Weldability Good with preheat/post-weld heat treatment Poor (needs preheat and stress relief)
Cost (casting + machining) High (forged or machined billets) 20 – 50 % lower (near-net shape)
Typical Uses High-strength shafts, pressure vessels, heavy structural components Crankshafts, pump housings, gearboxes, machinery frames

Ductile Iron vs. Aluminum and Bronze

Metric Aluminum Alloy (e.g., 6061-T6) Bronze (e.g., C93200) Ductile Cast Iron (DI)
Density (g/cm³) ~ 2.70 8.4 – 8.9 ~ 7.20
Tensile Strength (MPa) 290 – 310 ~ 350 400 – 900
Elongation (%) 12 – 17 % 10 – 15 % 3 – 18 %
Thermal Conductivity (W/m·K) ~ 205 ~ 50 – 100 35 – 50
Corrosion Resistance Excellent (anodized) Excellent (marine environment) Moderate (coating or alloying required)
Wear Resistance Moderate Very good (anti-friction) Good to excellent (depending on grade)
Cost (per kg) Moderate High (2–3× DI) Low to moderate
Machinability Excellent (Ra ~ 0.2–0.4 µm) Moderate Good (requires carbide tooling)
Typical Uses Aircraft structures, heat exchangers, consumer electronics Bearings, bushings, marine hardware Gears, suspension components, pump housings, engine blocks

When to Favor Ductile Cast Iron

  • Cyclic or High-Load Components: DI’s combination of tensile strength (≥ 500 MPa), fatigue endurance (≥ 200 MPa), and damping makes it ideal for crankshafts, gears, and suspension arms.
  • Near-Net-Shape Complexity: Sand or shell casting ductile cast iron reduces machining allowances by 30–50% compared to steel, lowering overall part cost.
  • Cost-Sensitive Medium-Volume Production: When steel forgings or machined aluminum incur excessive costs, ductile iron offers a balance of performance and economy.
  • Corrosive or Wear-Resistant Fittings: With suitable coatings or alloying, ductile cast iron pipelines and pump housings endure decades in aggressive environments.

When Other Materials Prevail

  • Ultra-Lightweight Requirements: In aerospace fuselage skins, electric vehicle bodies, or portable electronics, aluminum or magnesium alloys deliver unmatched weight savings.
  • Extreme Corrosive Environments: Splash zones, chlorinated process lines,
    or acidic drainage often demand stainless steels (e.g., 316, duplex) whose passive films surpass DI’s coated or alloyed barriers.
  • High-Temperature Service (> 350 °C): In turbine components or exhaust manifolds,
    nickel-based superalloys or heat-resistant steels (e.g., 17-4 PH) sustain strength where ductile cast iron would suffer creep.
  • Maximum Toughness and Weldability: Structural steel beams and plated pipelines remain preferred when forging, welding, or cold-forming require consistent, documentable performance.

11. Conclusion

Ductile cast iron stands out as a versatile, cost-effective engineering material.

Its spheroidal graphite microstructure delivers a rare blend of high tensile strength, substantial ductility, and excellent fatigue life.

Manufacturers can cast near-net shapes, minimize subsequent machining, and tailor properties through heat treatment, most notably in the form of austempered ductile iron (ADI).

Despite modest corrosion vulnerability, ductile iron’s recyclability, damping capacity,

and a broad range of standardized grades render it indispensable across automotive, pipeline, agricultural, energy, and consumer markets.

At DEZE, we stand ready to partner with you in leveraging these advanced techniques to optimize your component designs, material selections, and production workflows.

ensuring that your next project exceeds every performance and sustainability benchmark.

Contact us today!

 

FAQs

What distinguishes ductile cast iron from gray cast iron?

Ductile cast iron (DI) contains spheroidal (nodular) graphite rather than the flake graphite found in gray iron.

Those spherical nodules blunt crack propagation, yielding significantly higher tensile strength (400–900 MPa) and elongation (3–18 %) compared to gray iron’s 200–300 MPa and < 2 % elongation.

What machining considerations apply to ductile iron?

Ductile cast iron machines similarly to carbon steel but requires carbide tooling due to its high-carbon nodules.

Recommended cutting speeds range from 150–250 m/min, with feeds of 0.1–0.3 mm/rev.

Proper coolant use prevents built-up edge. High-hardness or ADI grades may require slower speeds or ceramic tools to avoid premature wear.

How does ductile iron compare in cost to alternative materials?

  • Ductile iron Vs. Gray Iron: Ductile cast iron raw material costs ~ 10–20 % higher.
    However, reduced wall thickness and machining allowances often yield total part costs 20–30 % lower in strength-critical applications.
  • Steel Vs. Ductile iron: Ductile iron castings frequently cost 20–50 % less than equivalent steel forgings or heavy-machined components.
  • Aluminum/Bronze Vs. Ductile iron: Ductile iron is less expensive per kg than bronze (2–3× higher cost) and, although heavier than aluminum,
    offers far greater strength, fatigue life, and lower material cost when weight is not the primary concern.
Scroll to Top